BOHUASend your drawing

Engineering guide

Draft Angle for Aluminum Casting

For aluminum walls over 25 to 40 mm (0.98 to 1.57 in) deep, ISO 8062-3:2023 lists 2.5° outside and 3.5° inside at grade DA for permanent molds, which include tilt-pour and low-pressure dies. Machine-molded sand gets 2.0° and 2.4°. For high-pressure die casting at that depth, NADCA's general note uses at least 1° outside and 2° inside. The one-side offset is depth × tan(angle).

On this page
  1. What draft angle does an aluminum casting need?
  2. Why do gravity and tilt-pour molds need more draft than die casting?
  3. How do you calculate draft angle and offset?
  4. How much machining stock does draft take on a 40 mm pump housing wall?
  5. How do you dimension a draft angle on a casting drawing?
  6. How does Bohua set draft on your part?
  7. Questions about aluminum casting draft

What draft angle does an aluminum casting need?

Use more draft on inside walls than on outside walls, and a larger angle on shallow walls than on deep ones. The table gives starting values per side for smooth walls over 25 to 40 mm (0.98 to 1.57 in) deep. In this table, permanent molds take the most draft and high-pressure dies the least.

Starting draft per side for walls over 25 to 40 mm (0.98 to 1.57 in) deep. ISO values cover all cast metals; NADCA values are for aluminum die castings.
Casting processOutside wall (°)Inside wall or core (°)Basis
Sand casting, machine molded2.0 (DA) / 2.7 (DB)2.4 (DA) / 3.3 (DB)ISO 8062-3:2023, Table 3
Sand casting, hand molded2.2 (DA) / 3.0 (DB)2.9 (DA) / 4.1 (DB)ISO 8062-3:2023, Table 2
Gravity permanent mold2.5 (DA) / 3.2 (DB)3.5 (DA) / 4.1 (DB)ISO 8062-3:2023, Table 4
Tilt-pour permanent mold2.5 (DA) / 3.2 (DB)3.5 (DA) / 4.1 (DB)ISO 8062-3:2023, Table 4 (permanent mold starting point)
Low-pressure permanent mold2.5 (DA) / 3.2 (DB)3.5 (DA) / 4.1 (DB)ISO 8062-3:2023, Table 4 (permanent mold starting point)
High-pressure die casting1 minimum (general note); formula: 0.96 at 25 mm (0.98 in) to 0.76 at 40 mm (1.57 in)2 minimum (general note); formula: 1.92 at 25 mm to 1.52 at 40 mmNADCA S-4A-7-15 general note and formula

Sources: ISO 8062-3:2023, Tables 2–4, and the North American Die Casting Association's 2015 Product Specification Standards for Die Castings (9th edition), S-4A-7-15. NADCA lists a 2024 edition; this guide used the 2015 text.

ISO lists two grades, DA and DB. In this height band, DA gives the smaller angles. This guide treats DB as a starting choice when the part has room for more taper. Tilt-pour and low-pressure dies are permanent molds, so their rows start from the permanent mold values. At Bohua, the die design review sets their final angle. NADCA's general note covers castings with most features at least 25.4 mm (1 in) deep. Confirm the minimum with the foundry before the tool is cut.

The angle drops as walls get taller. For a permanent mold at grade DA, ISO 8062-3:2023 Table 4 lists 2.8° outside for walls over 16 to 25 mm (0.63 to 0.98 in) deep and 1.8° for walls over 63 to 100 mm (2.48 to 3.94 in). The 2023 edition added these draft tables for hand-molded sand, machine-molded sand, permanent mold, pressure die and investment casting.

Cast-in texture. Set the draft for a cast-in texture per location, texture depth and pull direction in the drawing review. NADCA's die casting design guide allows stipples and grain to be cast in when the textured face is generally perpendicular to the direction of die draw. It also notes that detailed patterns reduce die life. On a side wall, texture needs extra draft, and published shop guides do not agree on how much. NADCA's draft formula does not cover cast lettering, logos or engraving, so review those features one by one.

Source: NADCA Product Design for Die Casting, 7th edition, 2015, Section 3.4.

Why do gravity and tilt-pour molds need more draft than die casting?

The standards show the gap. For walls over 25 to 40 mm deep, ISO 8062-3:2023 lists 2.5° outside for a permanent mold at grade DA, while NADCA's die casting general note uses a 1° minimum. A gravity or tilt-pour die is a permanent mold. It opens around a solid casting, and the part slides along each wall as it comes out. Permanent molds also carry a refractory coating that helps the casting release, and enough draft helps keep that coating intact.

The tilt angle during pouring does not set the draft. The mold-opening and core-pull directions do. Inside walls need the most draft, because the casting shrinks away from outside walls and onto cores as it cools. NADCA recommends twice as much draft on inside walls for this reason. Check the pull direction and order for each metal core.

In sand casting, the draft on a pattern lets it lift out of the sand before pouring. The foundry later breaks the mold away from the casting. Sand cores do the same job inside a permanent mold: a sand core can form a hole or passage that cannot take draft, and it breaks out after casting. That route is called semi-permanent mold. The core box still needs draft so the core can be released.

Steel casting die on an angled tilting frame
Permanent mold on a tilt-pour frame

See the tilt-pour permanent mold process for the pouring arrangement and the aluminum gravity casting design guide for related geometry checks. The permanent mold casting guide explains where the process fits.

How do you calculate draft angle and offset?

Multiply the draw depth by the tangent of the draft angle to get the single-side offset. Measure the depth along the pull axis and the angle from a line parallel to it. Set your calculator to degrees.

Single-side offset = draw depth × tan(draft angle)

To find the angle from a measured offset, reverse it: Draft angle = arctan(offset ÷ draw depth). A wall that moves 1.0 mm over 40 mm has arctan(0.025) = 1.43° of draft.

Single-side offset in mm (in) for a straight wall at the stated draw depth
Draft angle (°)10 mm (0.39 in)25 mm (0.98 in)50 mm (1.97 in)100 mm (3.94 in)
0.50.09 (0.003)0.22 (0.009)0.44 (0.017)0.87 (0.034)
1.00.17 (0.007)0.44 (0.017)0.87 (0.034)1.75 (0.069)
1.50.26 (0.010)0.65 (0.026)1.31 (0.052)2.62 (0.103)
2.00.35 (0.014)0.87 (0.034)1.75 (0.069)3.49 (0.137)
3.00.52 (0.021)1.31 (0.052)2.62 (0.103)5.24 (0.206)

Double the single-side offset to find the change in width when opposing walls have equal, symmetric tapers. For a round feature with uniform draft, the single-side offset is the change in radius. Compare the diameter at each end if a bore or an outside pilot must clear a mating feature.

How does the NADCA die casting draft formula differ?

NADCA's standard draft formula gives a starting angle for conventional high-pressure die casting. In the 2015 inch-based formula, draft distance D = √L / C and angle in degrees = 57.2738 / (C√L), with draw depth L in inches. For aluminum, C = 60 for an outside wall and C = 30 for an inside wall. NADCA prints this constant; using 180/π (57.2958) instead changes these results by less than 0.01°. The calculated angle drops as the depth increases, even as the offset grows.

For a cored hole, NADCA gives the total draft on the diameter, with C = 20 for aluminum. A hole 25.4 mm (1 in) deep tapers √1 ÷ 20 = 0.050 in (1.27 mm) on the diameter. Keep that total separate from a per-side wall callout.

How much machining stock does draft take on a 40 mm pump housing wall?

A cast aluminum pump housing wall 40 mm (1.57 in) deep with 1.5° of draft moves 1.05 mm (0.041 in) on one side: 40 × tan(1.5°) = 1.05 mm. If you machine that wall straight, the stock changes by 1.05 mm from one end to the other. At the ISO permanent mold grade DA value of 2.5° for this height, the same wall moves 1.75 mm (0.069 in).

Put the minimum stock at the low-metal end. Say the cut needs at least 1.0 mm of stock everywhere, an example value rather than a standard. The cast wall then carries 1.0 mm at the low-metal end and 2.05 mm at the other end, before casting tolerance. At 2.5°, the high end carries 2.75 mm. For required machining allowance (RMA) grades, see the aluminum casting shrinkage allowance guide.

Keep the cast and finished surfaces in one section view to spot thin corners or interrupted cuts. Put the machining datum where the inspection and fixture plans can reproduce it. Use the ISO 8062 casting tolerance guide to separate the tolerance band from the nominal taper.

How do you dimension a draft angle on a casting drawing?

Show the angle per side, the pull direction, the plane where the size applies, and whether draft adds or removes metal. If the drawing says nothing, expect the foundry to add draft.

  1. Mark the draw direction. Put an arrow on the section view. Add a separate arrow for a slide or retractable core that moves in a different direction. If the direction matters, show it; otherwise the foundry chooses it from the parting line.
  2. Locate the controlling size. State where the width or diameter applies, such as the far end or the parting plane. Where a parting line splits a wall, the longer portion sets the draft.
  3. Say whether draft adds or removes metal. If the drawing is silent, expect added draft. That is standard foundry practice under the Aluminum Association's Standards for Aluminum Sand and Permanent Mold Castings (15th edition, 2008), section E4. With added draft, the drawn size is the minimum-metal size, so the stock you draw is the minimum stock. Mark “draft removes material” only where extra metal would break a fit or a clearance. On a cored bore, added draft makes the bore smaller.
  4. Separate cast and machined notes. Identify cleanup surfaces, local stock and finished dimensions. Set a minimum as-cast wall where a cut passes close to a core.

An example note for the wall above is Outer wall: 1.5° draft per side. Diameter applies at the far end. Draft adds material toward the parting plane. Pair it with a view that shows the direction, and put local exceptions on the affected feature.

On an ISO drawing, the general tolerance note can call up an ISO 8062-3:2023 draft grade. The table angles then apply to every feature without its own draft callout, and to the longer feature in the direction of taper. ISO applies them as a tolerance that widens along the feature, not as a change to the nominal shape (Clause 6). Taper plus (TP) applies unless the drawing says otherwise, and features with a maximum material requirement take taper minus (TM) (Clause 5). If you model draft into the CAD shape, say so on the drawing.

For an RFQ, send the current CAD model and the controlling drawing. Follow the casting drawing requirements when you mark the finished surfaces and datums.

How does Bohua set draft on your part?

For tilt-pour and low-pressure parts, Bohua starts from the permanent mold values above and sets the final draft in its die design review. Bohua designs and makes its molds in-house. Tool design uses UG and SolidWorks, and casting simulation uses AnyCasting.

Bohua casts aluminum in-house by four processes: gravity casting including tilt-pour, low-pressure casting, die casting on two machines rated at 280 t and 450 t, and sand casting. Ten hot-box core shooters support sand cores, including cores used for some tilt-pour parts. Bohua casts and machines aluminum pump housings, valve bodies and impellers in batch production.

At Bohua

The drawing review is free. Send the 2D drawing and the 3D model. Mark the faces you will machine, the bores formed by cores and any textured zones. Our engineers check which casting process suits the part and suggest where the design could change, once we know what the part must achieve. You decide which changes go into the drawing. Many of the parts we cast today went into production with changes we proposed. Tooling, samples and parts are quoted as usual. First article takes 5–6 weeks from drawing confirmation. Use the aluminum casting RFQ page or write to linda@ningbobohua.com.

Core shooting machines with sand cores stacked on a rack
Hot-box core shooters for sand cores

Questions about aluminum casting draft

Can I call out zero draft on a machined surface?

Yes, on the finished face. The cast blank still needs draft and enough stock along the cut. If the as-cast face must also be straight, ask the foundry to review that feature before the parting line is fixed.

Do inside and outside walls need the same draft?

No. Inside walls need more, because the casting shrinks onto cores as it cools. NADCA recommends twice as much draft on inside walls. For permanent mold walls over 25 to 40 mm deep, ISO 8062-3:2023 lists 3.5° inside against 2.5° outside at grade DA.

Is the draft angle the included angle?

No. Draft is called out per side, from the pull direction. The included angle between two equally drafted walls is twice that. Write “per side” on the drawing.

Does draft change a machined diameter?

No. Draft changes the as-cast diameter along the pull. The finished diameter follows the machining callout. Check that the blank covers the full finished size at the low-metal end.

Does texture added after casting need extra draft?

No. Release depends on the surface that leaves the mold. A texture cast into a side wall does need extra draft, set at drawing review.

What is the minimum draft angle for casting?

It depends on the process. For aluminum die casting, NADCA's general note uses at least 1° outside and 2° inside on walls over 25 to 40 mm deep. NADCA's precision tolerances go lower, generally to 0.75° per side on inside walls and half that on outside walls. That needs extra precision in die construction or special production control, so NADCA says to specify it only when necessary. For sand and permanent molds, the smaller ISO 8062-3:2023 grade, DA, is in the first table.

Send your drawing for a free drawing review

Include the 2D drawing and 3D model. Mark the pull direction, controlling dimensions and faces to machine. Submit the RFQ details, then email your drawing for review.