Aluminum casting shrinkage allowance is the amount a pattern or die is made oversize so the cooled casting reaches its target size. SAE J452 lists 1.30% (5/32 in/ft) for average sand castings in A356.0, A357.0 and 319.0. Producer data give 0.8–1.1% for A356-type AlSi7Mg alloys in gravity permanent molds, and NADCA lists 0.6% for die-cast 380. Final values are set per project from tooling experience and first-article measurement.

On this page
  1. What aluminum casting shrinkage percentage should you use?
  2. Is shrinkage allowance the same as solidification shrinkage?
  3. Why can two features in one casting shrink differently?
  4. How do you calculate mold size from shrinkage allowance?
  5. How do you specify shrinkage and machining allowance on a drawing?
  6. How does Bohua set shrinkage allowance on new tooling?
  7. Questions about aluminum casting shrinkage

What aluminum casting shrinkage percentage should you use?

Start from a published value for your alloy and process. SAE J452 lists 1.30% (5/32 in/ft) for average sand castings in A356.0, A357.0 and 319.0. Producer data for AlSi7Mg alloys, the European counterparts of A356 and A357, give 0.8–1.1% in a gravity permanent mold. NADCA lists 0.6% for die-cast 380. In Rheinfelden's table, every alloy listed for all three processes takes the most allowance in sand and the least in high-pressure die casting.

Linear shrinkage allowance for aluminum tooling: published starting values (%)
AlloySand casting (%)Gravity permanent mold (%)High-pressure die casting (%)
A356.0 and A357.01.30 (SAE J452). 1.1–1.2 for AlSi7Mg0.3 and AlSi7Mg0.6 (Rheinfelden).0.8–1.1 for AlSi7Mg0.3 and AlSi7Mg0.6 (Rheinfelden)Not listed for die casting in SAE J452. Set per project if proposed.
319.01.30 (SAE J452)No published value found. The SAE 1.30% applies to sand castings only.Not listed for die casting in SAE J452
380.0 and A380.0Die-casting alloy in SAE J452Die-casting alloy in SAE J4520.6 for 380 (NADCA). No separate A380.0 value found.
ADC12 (JIS H 5302)Die-casting alloyDie-casting alloyNo published value found. NADCA cross-references ADC12 to 383.

Where no published value was found, the allowance is set per project from tooling experience and first-article measurement. Tilt-pour and low-pressure dies are permanent molds, so the gravity permanent mold column is their starting point too. The final value for each feature comes from the die design review.

Sources: SAE J452_201801, Table 2A, Pattern Shrinkage Allowance column and note 2, with casting types from Table 1. SAE stabilized J452 in January 2018; its last technical revision was December 2003. Rheinfelden Alloys, Primary Aluminum Casting Alloys, edition 08/2018, physical properties table. NADCA, Product Specification Standards for Die Castings, 9th edition (2015), Competitive Performance Chart, p. 3-41 (pattern shrinkage 0.006 in/in for 380 die cast), and alloy cross-reference, p. 3-42.

Across the aluminum sand alloys in SAE J452, the listed allowance runs from 0.83% (1/10 in/ft) for 520.0 and 535.0 to 1.56% (3/16 in/ft) for 705.0 through 713.0. Most alloys, including A356.0, A357.0 and 319.0, sit at 1.30%. SAE adds that the requirement varies with the intricacy of the design and its dimensions.

The permanent mold values come from Rheinfelden's data for AlSi7Mg0.3 (EN AC-42100) and AlSi7Mg0.6 (EN AC-42200), the closest European grades to A356 and A357. Confirm the actual alloy against the drawing. For the metal mold process and its design inputs, see the permanent mold casting guide and the A356 material page.

Is shrinkage allowance the same as solidification shrinkage?

No. Shrinkage allowance is a linear correction, near 1%, built into the tool. Solidification shrinkage is the volume the metal loses as it freezes, and risers and feeding must make it up. Shrinkage porosity is the void left where that feeding fails.

Three shrinkage terms and where each belongs
TermWhat it isTypical size for aluminumWhere it is handled
Pattern or die shrinkage allowanceLinear oversize built into the pattern, die or core box0.6–1.3% in the table aboveTool design, then correction after first-article measurement
Volumetric solidification shrinkageVolume lost as the liquid metal freezesLiquid aluminum is 6.5% less dense than solid aluminum. Silicon reduces the loss.Gating, risers and feeding
Shrinkage porosity or cavityVoids left where freezing metal was not fedNot a percentage. Judged by X-ray or sectioning in agreed zones.Feeding design, plus acceptance zones on the drawing

If a source quotes several percent of shrinkage for aluminum, it is describing volume. The linear values in the references above stay below 2%. SAE J452 keeps the two apart: its pattern allowance column is linear, and a separate column ranks solidification shrinkage, the volume decrease that risers must feed.

A correct external length can coexist with an internal shrinkage cavity. A sound part can also miss a dimension. Address both on the drawing where they affect function. See the casting porosity guide for defect mechanisms and inspection.

Sources: European Aluminium, Aluminium Automotive Manual, Cast alloys and products, version 2002, p. 12. SAE J452_201801, Table 2A, note 5. NADCA 2015 glossary, solidification shrinkage.

Why can two features in one casting shrink differently?

The mold and cores hold some features while others shrink freely. A free length can shorten far more than a span held between rigid mold sections or around a core. Wall thickness, core layout, mold temperature and the time of release also change the result.

A 2024 study of a U-shaped AlSi7Mg0.3 casting in a gravity permanent mold shows the size of the effect. The free end shrank 1.14% at every demolding temperature tested. The inner length between the legs of the U, which the mold held until release, shrank only 0.07% to 0.26%, depending on the demolding temperature. One factor for the whole part can therefore miss a restrained feature.

Source: N. Wolff, S. Gor, U. Vroomen and A. Bührig-Polaczek, Materialwissenschaft und Werkstofftechnik 55(1), 33–39 (2024), Section 3.2, doi:10.1002/mawe.202300133.

How feature type changes contraction, and what to check on first castings
FeatureTypical behaviorCheck on first castings
Free outside lengthShrinks freely: 1.14% at the free end in the 2024 studyLength against the as-cast target
Span held by the mold or a coreShrinks less while restrained: 0.07–0.26% in the same studySpan length and the wall next to the core
Core-formed bore or passagePosition follows core location and any core shiftMachining stock all around the bore
Thin flange beside a heavy sectionCools at a different rate and can bowFlatness or profile, not only length

After first castings, the toolmaker compares measured features with the approved as-cast targets. A consistent size error may call for a cavity or insert change. A local error may call for work at the core, a change to the cooling setup or a review of the part shape. Measure against the agreed datums and record the inspection stage. If acceptance applies after heat treatment, check again after heat treatment. Repeat the measurements after each tool change before releasing production dimensions.

How do you calculate mold size from shrinkage allowance?

Multiply the as-cast target by (1 + allowance). In this worked example, a 200 mm (7.874 in) as-cast length in an A356 permanent mold at an assumed 1.0% needs a 202.00 mm (7.953 in) cavity. The 1.0% is an assumed input inside the 0.8–1.1% producer range for AlSi7Mg alloys.

Cavity length = as-cast target × (1 + allowance / 100)

200 mm × 1.010 = 202.00 mm

Cavity length for a 200 mm (7.874 in) as-cast length at the published values on this page
Allowance (%)BasisCavity length, mm (in)Oversize, mm (in)
0.6Die-cast 380, NADCA201.20 (7.921)1.20 (0.047)
0.8Low end, AlSi7Mg gravity permanent mold201.60 (7.937)1.60 (0.063)
1.0Worked-example assumption202.00 (7.953)2.00 (0.079)
1.1High end, AlSi7Mg gravity permanent mold202.20 (7.961)2.20 (0.087)
1.3A356.0 sand, SAE J452202.60 (7.976)2.60 (0.102)

Within the permanent mold range alone, the cavity moves by 0.60 mm (0.024 in). Compare that with the tolerance on the dimension before you accept one factor for the whole part.

Add machining stock before you scale. If 200 mm is a finished length with 2.0 mm (0.079 in) of stock on each end, the as-cast target is 204.00 mm (8.031 in). At 1.0%, the cavity is 204.00 × 1.010 = 206.04 mm (8.112 in).

Ask how your toolmaker defines the percentage. The formula above applies it to the casting size, as NADCA's contraction factor does: a multiplier on casting dimensions that gives die dimensions. If 1.0% instead means contraction measured from the cavity, divide: 200 ÷ 0.990 = 202.02 mm (7.954 in). NADCA's factor also covers the different thermal expansion of die steel and alloy and the die's operating temperature. Compare a cold tool report with a cooled part only on the same basis.

Source: NADCA, Product Specification Standards for Die Castings, 9th edition (2015), glossary, contraction factor, p. 10-12.

How do you specify shrinkage and machining allowance on a drawing?

Draw the part at finished nominal size and let the foundry apply shrinkage to its tooling. On the drawing, state the delivery condition, the controlling as-cast dimensions, each machined face with its stock, and the inspection datums.

ISO 8062-3:2023 (edition 2) treats machining allowance separately from casting tolerance. The required machining allowance (RMA) is the stock left for machining. Its grade (RMAG) is used to select that stock. Shrinkage allowance belongs to the tool, not to the part drawing. See the ISO 8062 casting tolerance guide for grade selection and drawing conventions.

  1. Model basis. Add a note such as “Model at finished nominal size. Foundry applies shrinkage allowance. Do not scale.”
  2. Machining stock. Mark each machined face and give its stock, for example “2.0 mm stock on faces marked M.”
  3. Inspection state. Say when and where as-cast dimensions are checked, for example “Inspect as-cast dimensions after T6, at room temperature, from datums A-B-C.”
  4. Restrained features. Flag core-formed bores and spans held by inserts for first-article checks.

If a flange arrives with stock for face machining, size the as-cast envelope first. Mark the finished face and show where the stock sits. The foundry can then size the cavity for the blank, and the machine shop can check that the whole face cleans up. Draft on the same faces changes the stock as well. See the draft angle guide for aluminum castings.

In an RFQ, send the as-cast and finished models if both exist, each with its revision. Mark sealing faces, locating bores and other critical fits. State whether first-article measurements apply before or after heat treatment. Give the rough casting weight and the finished weight if you have them. If the foundry builds the cast model, ask for its proposed as-cast envelope before tooling approval.

How does Bohua set shrinkage allowance on new tooling?

At Bohua

Tilt-pour and low-pressure dies are permanent molds, so at Bohua we start from the permanent mold references above. The final allowance for each feature is set in our die design review from tooling experience, and first-article measurement confirms it.

We run four casting processes in-house: gravity casting, including tilt-pour casting; low-pressure casting, in-house since 2014; die casting on a 280 t and a 450 t machine; and sand casting. We use A356 and ZL114 for gravity and tilt-pour casting. Die-casting alloys follow the customer's specification, and ADC12 is a common choice. We cast and machine aluminum pump housings, valve bodies and impellers in batch production.

We design and make our dies in-house, using UG and SolidWorks for die design and AnyCasting for casting simulation. From drawing confirmation to first article takes 5–6 weeks. Dimensional inspection uses Hexagon Global S and NANO Metrology coordinate measuring machines and a handheld 3D scanner. Casting, T5 and T6 heat treatment, CNC machining and inspection share our site of about 16,300 m².

Our as-cast tolerance is CT8. Selected demanding as-cast dimensions can reach about DCTG 6 under ISO 8062-3. Key machined features can reach ±0.02 mm where the drawing, feature and datum scheme allow.

The drawing review is free. Our engineers check which casting process suits the part and suggest where the design could change, once we know what the part must achieve. You decide which changes go into the drawing. Use the casting RFQ page to send the finished drawing, the alloy specification and the surfaces that need machining.

Bridge coordinate measuring machine in a dimensional inspection room
Coordinate measuring machine for dimensional inspection
Steel casting molds on blue storage racks
Casting molds stored on racks

Questions about aluminum casting shrinkage

What is the shrink rate of cast aluminum?

For pattern and die sizing, SAE J452 lists 1.30% (5/32 in/ft) for common sand-cast alloys such as A356.0, A357.0 and 319.0. Producer data give 0.8–1.1% for A356-type alloys in a gravity permanent mold, and NADCA lists 0.6% for die-cast 380. The volume change on freezing is a separate number: liquid aluminum is 6.5% less dense than solid aluminum. Risers and feeding make up that volume, not mold scaling.

Can I use the same shrinkage percentage for sand and permanent mold?

No. Rheinfelden lists the same AlSi7Mg alloys at 1.1–1.2% in sand and 0.8–1.1% in a gravity permanent mold, and SAE J452 lists 1.30% for average A356.0 sand castings. Start from one published source and note which one. A rigid metal mold and a sand mold let the casting move differently as it cools. Metal and sand cores also restrain the same feature differently.

Does shrinkage allowance cover a machined bore?

No. Shrinkage allowance only sizes the tool. Machining stock is a separate allowance. Set the as-cast bore from the finished diameter and its stock first, then apply the factor the toolmaker uses for that feature. Check that stock remains all around the bore after any core shift.

Will enlarging the mold prevent shrinkage porosity?

No. Mold scaling corrects size, not soundness. Gating, risers and the freezing sequence control shrinkage porosity. If a zone must be sound, define the zone and the acceptance method in the RFQ.

Should I scale my CAD model for shrinkage before I send it?

No. Send the part at nominal size and state the delivery condition. The foundry builds shrinkage and machining stock into its tooling model. If you send a tooling model, say which allowances it already contains.

Send your drawing for a free drawing review

Include the finished geometry, casting alloy, inspection stage and faces that require machining. Submit the RFQ details, then email your drawing for review.

Send your drawing →

Linda

Export Sales

linda@ningbobohua.com

Ningbo, Zhejiang, China