BOHUASend your drawing

Engineering guide

A356 vs A357 Aluminum Casting: Chemistry, Minimum Properties and Equivalent Grades

A357 is A356 with more magnesium (0.40–0.7% vs 0.25–0.45%) and, as registered, 0.04–0.07% beryllium. In the SI table of ASTM B108/B108M-19, A357.0-T61 permanent-mold test bars have minimums of 310 MPa tensile and 250 MPa yield, against 260 and 180 MPa for A356.0-T61, while minimum elongation falls from 4% to 3%. The closest equivalents are EN AC-42200 and ZL114A for A357, and EN AC-42100 and ZL101A for A356.

Gravity casting machines on the left, racks of sand cores in the middle and a row of holding furnaces under fume hoods
On this page
  1. A356 vs A357: the quick answer
  2. How do A356 and A357 differ in chemistry?
  3. How much stronger is A357 in ASTM, EN and GB?
  4. A357 and A356 equivalents: EN, GB and JIS grades
  5. When is A357 worth it?
  6. How to call out A356 or A357 on a drawing
  7. A356 and ZL114 at Bohua
  8. A356 vs A357: buyer questions
  9. Sources

A356 vs A357: the quick answer

Use A356 unless a zone needs more yield than A356 can show on your test basis. Then A357 is the step up, if 3% elongation is acceptable. Under ASTM B108 that line is 180 MPa (26 ksi) for A356.0-T61, on test bars and on specimens cut from the casting. Under EN 1706 permanent-mold T6 it is 210 MPa for EN AC-42100 test bars.

A356 vs A357 at a glance
ItemA356 (A356.0)A357 (A357.0)
Magnesium, %0.25–0.450.40–0.7
Beryllium, %No addition; counts as an "other" element, 0.05 max0.04–0.07 (E357.0 and F357.0: 0.002 max)
ASTM B108/B108M-19 SI table, T61 test bars: tensile / yield / elongation260 / 180 MPa / 4%310 / 250 MPa / 3%
Same table, specimens cut from a designated area230 / 180 MPa / 4%315 / 250 MPa / 3%
EN 1706 permanent mold, T6 test barsEN AC-42100: 290 / 210 MPa / 4%EN AC-42200: 320 / 240 MPa / 3%
Closest grade in GB/T 1173-2013ZL101AZL114A
Choose it whenYield needed is at most 180 MPa (B108) or 210 MPa (EN 1706), or elongation must exceed 3%Higher yield is needed, and 3% elongation is acceptable

Sources: Pink Sheets (August 2025); ASTM B108/B108M-19, Table 3 (B108/B108M-25 is active); EN 1706:2020+A1:2021, Table 3; GB/T 1173-2013, Table 1. Property values are minimums; ASTM checks yield only when the order asks.

How do A356 and A357 differ in chemistry?

Both alloys have 6.5–7.5% silicon. A357 adds magnesium (0.40–0.7% against 0.25–0.45%), needs at least 0.04% titanium and, as registered, carries 0.04–0.07% beryllium. The extra magnesium raises yield and lowers elongation.

Registered composition limits, % by mass (Aluminum Association, August 2025)
ElementA356.0 (castings)A356.2 (ingot)A357.0 (castings)E357.0 (castings)F357.0 (castings)
Silicon6.5–7.56.5–7.56.5–7.56.5–7.56.5–7.5
Iron, max0.200.120.200.100.10
Copper, max0.200.100.20—0.20
Manganese, max0.100.050.100.100.10
Magnesium0.25–0.450.30–0.450.40–0.70.55–0.60.40–0.7
Zinc, max0.100.050.10—0.10
Titanium0.20 max0.20 max0.04–0.200.10–0.200.04–0.20
Beryllium——0.04–0.070.002 max0.002 max
Others, each / total, max0.05 / 0.150.05 / 0.150.05 / 0.150.05 / 0.150.05 / 0.15

A dash means no specific limit: the element then counts as an "other", 0.05% max each (Pink Sheets, footnote 12).

  • A356 vs A356.2. The digit after the point is the product form: .0 is castings, .1 and .2 are ingot. A356.2 ingot has tighter iron, copper, manganese and zinc limits and a higher magnesium floor. Your drawing names A356.0, the casting limits, even if the foundry melts A356.2 ingot.
  • Beryllium. Research ties the addition to iron phases: beryllium turns most of the plate-like β-Al5FeSi phase into the script-type π phase, and a 2018 study measured a higher quality index with 0.05% Be. IARC classifies beryllium and its compounds as carcinogenic to humans (Group 1). GB/T 1173-2013 bars beryllium in aluminum alloy products that contact food.
  • Iron. Iron is the most harmful impurity in Al-Si-Mg casting alloys. E357.0 and F357.0 cap it at 0.10%, half the A356.0 and A357.0 limit.

How much stronger is A357 in ASTM, EN and GB?

Every standard that lists both grades sets the A357 type higher on strength and equal or lower on elongation. The gap is largest in ASTM B108 and smallest in GB/T 1173.

Minimums: tensile / yield, MPa (ksi in the inch-pound row) / elongation, %; separately cast test bars unless noted
Standard, process, temperA356-type gradeA357-type grade
ASTM B108/B108M-19 Table 3 (SI), permanent mold, T61; elongation in 5DA356.0: 260 / 180 / 4A357.0: 310 / 250 / 3
Same, Table 2 (inch-pound), ksi; elongation in 2 in. or 4DA356.0: 38 / 26 / 5A357.0: 45 / 36 / 3
Same, Table 3, specimens cut from castings, designated areaA356.0: 230 / 180 / 4A357.0: 315 / 250 / 3
Same, no location designatedA356.0: 195 / 180 / 3A357.0: 285 / 215 / 3
ASTM B26/B26M-18 Table 4 (SI), sand, T6A356.0: 235 / 165 / 3.5A357.0: not listed
EN 1706:2020+A1:2021 Table 3, permanent mold (K) or low pressure, T6EN AC-42100: 290 / 210 / 4EN AC-42200: 320 / 240 / 3
EN 1706 Table 2, sand (S), T6EN AC-42100: 230 / 190 / 2EN AC-42200: 250 / 210 / 1
GB/T 1173-2013 Table 3, metal mold (J, JB)ZL101A, T6: 295 / not listed / 3ZL114A, T5: 310 / not listed / 3
GB/T 1173-2013 Table 3, modified sand (SB)ZL101A, T6: 275 / not listed / 2ZL114A, T5: 290 / not listed / 2

ASTM rows: B108/B108M-19 and B26/B26M-18, the latest editions checked for this page; B108/B108M-25 and B26/B26M-25 are active, so confirm against the edition on your order. ASTM keeps SI and inch-pound values separate. Cut-specimen rows cover sections up to 2 in. (about 50 mm).

  • GB T5 is not EN T5. In GB/T 1173-2013, T5 means solution treatment plus incomplete artificial aging. In EN 1706, T5 means controlled cooling from casting plus artificial aging.
  • Achievable values are closer. EN 1706 Annex B (informative) lists potentially achievable values on test pieces cut from permanent-mold or chilled sand castings: 300 / 240 MPa / 11% for EN AC-42100 and 315 / 240 MPa / 8% for EN AC-42200. It warns that they may need extra production measures and must be agreed with their zones. At that level the yield is equal, and the A357 type gives up three points of elongation.

A357 and A356 equivalents: EN, GB and JIS grades

No grade is an exact equivalent. The closest matches share the silicon and magnesium windows but differ in impurity limits, beryllium, titanium and the tempers they are tested in.

Closest grades and the differences to check before approval
FamilyAA / ASTMEN 1706GB/T 1173-2013JISCheck before you accept it
A356A356.0 castings; A356.2 ingotEN AC-42100, AlSi7Mg0.3ZL101A, ZAlSi7MgAAC4CHEN caps copper at 0.05% and zinc at 0.07%. GB requires titanium at 0.08–0.20%.
A357A357.0 with Be; E357.0 and F357.0 with Be 0.002% maxEN AC-42200, AlSi7Mg0.6ZL114A, ZAlSi7Mg1ANone listedEN 1706 pairs 42200 with 357.0, not A357.0, and adds no Be. ZL114A allows Be up to 0.07% and Mg up to 0.75%, and GB tests it as T5.

EN 1706:2020+A1:2021, Annex D (informative), pairs EN AC-42100 with A356.0 and AC4CH, and EN AC-42200 with 357.0. The other entries come from comparing composition limits in the Pink Sheets and GB/T 1173-2013, Tables 1 and 2.

Treat a cross-reference as a starting point for approval, not as permission to substitute. GB/T 1173-2013 lists the A357-type grade as ZL114A (ZAlSi7Mg1A). A drawing that says only ZL114 should name the standard and edition; the ZL114 material page lists what to confirm.

When is A357 worth it?

Choose A357 when the yield you must prove is above what A356 can show on your test basis, and the part cannot simply get thicker.

  • A section that cannot grow. When a thin wall or a fixed envelope rules out more metal, the alloy is the remaining lever.
  • A specification that names it. Some customer and industry specifications call for A357, EN AC-42200 or ZL114A by name.

What you give up or must manage:

  • Elongation. Minimum elongation is lower for the A357 type on ASTM B108 test bars and in EN 1706. In GB/T 1173-2013 it is the same, 3% in metal mold, but the two grades are listed in different tempers.
  • Beryllium. If your restrictions exclude it, look at E357.0 or F357.0 (Be 0.002% max) or EN AC-42200 (no Be addition; Be counts as an "other", 0.03% max). B108/B108M-19 rates E357.0-T61 like A357.0-T61 but lists F357.0 only as T6, with no yield minimum. Get any change approved by the design authority.
  • Ingot supply. Ask which ingot the foundry can buy. One primary producer's 2019 catalog lists this family only as 357.1, F357.1 and F357.2, none with a beryllium addition.

What does not change: EN 1706 Annex C rates EN AC-42100 and EN AC-42200 the same for fluidity, hot-tear resistance and pressure tightness. It also gives both the same rotating-bending fatigue range, 80–110 MPa (12–16 ksi) up to 10⁷ cycles. A357 buys static strength, not castability.

Worked example: does this zone need A357?

A suspension bracket's stress check calls for a minimum yield of 200 MPa (29 ksi) in its mounting boss. The figures are illustrative; the suspension bracket RFQ checklist lists what to send with such a part.

  1. ASTM B108 test bars. A356.0-T61 gives 180 MPa, below 200. A357.0-T61 gives 250 MPa, 25% above.
  2. ASTM B108 specimens cut from the boss. With the boss marked on the drawing, B108 keeps yield at 180 MPa for A356.0-T61 and 250 MPa for A357.0-T61. With no location marked, it is 180 and 215 MPa.
  3. EN 1706 test bars, permanent mold T6. EN AC-42100 gives 210 MPa, 5% above. EN AC-42200 gives 240 MPa, 20% above.
  4. EN 1706 specimens cut from the casting. EN 1706 leaves these values to agreement and notes that strength in the casting may fall to 70% of the bar values: 147 and 168 MPa. Neither reaches 200, so agree 200 MPa for the boss, mark the location and verify it on first articles.

Result: on a B108 order, only A357 covers 200 MPa, on bars and in the boss. On an EN 1706 order, A356 passes on bars with a 5% margin, but the boss value must be agreed for either alloy. If you are still choosing between a machined part and a casting, read billet vs cast aluminum.

How to call out A356 or A357 on a drawing

A complete callout names six things: standard and edition, grade, casting process, temper, a yield requirement if the design uses yield, and the test basis with location.

  1. Standard and edition. For example ASTM B108/B108M-25, EN 1706:2020+A1:2021 or GB/T 1173-2013. Under ASTM, write B108M if you want the SI values; otherwise castings are supplied to the inch-pound values.
  2. Grade, process and temper. EN writes them as one string, such as EN 1706 AC-42100-K-T6, where K means permanent mold. In ASTM terms: A356.0-T61, permanent mold, to B108.
  3. Yield, if you need it. ASTM B108 evaluates yield strength only when the contract or purchase order asks for it. If your stress check uses yield, write the yield requirement into the callout.
  4. Test basis. Separately cast test bars, poured with the parts and heat treated with them, or specimens cut from the casting after heat treatment.
  5. Location and frequency. For cut specimens, mark the zone on the drawing and state how many per lot. Without a marked zone, B108 takes specimens where the wall thickness changes significantly.
  6. Values. Test bars use the standard's minimums. For cut specimens, B108 has A356.0 and A357.0 rows and applies 75% of strength and 25% of elongation to other alloys; B26 applies that rule to sand castings. EN 1706 allows strength down to 70% of the bar values and elongation up to 50% lower in some locations. GB/T 1173-2013 refers to GB/T 9438. Write any zone value on the drawing.

Test bars check the melt and the heat treatment. They do not prove the strength of a thick boss or a thin rib. See the guide to ASTM, ISO and IATF scope and the T6 heat treatment guide, which covers the batch records that tie test bars to parts. For A356 evidence, see the A356 material page and the A356 properties and testing guide.

A356 and ZL114 at Bohua

At Bohua

We cast A356 and ZL114 on our gravity and tilt-pour lines, with T5/T6 heat treatment in-house. Low-pressure casting, die casting on 280 t and 450 t machines, and sand casting are also done in-house. We degas each melt for 15 to 20 minutes with the rotor at 480 to 520 rpm. A melt goes to production only after two checks pass: a sample taken with our vacuum hydrogen analyzer shows a slightly concave surface and is essentially free of pores when cut, and our Oxford optical emission spectrometer confirms the chemistry. Tensile tests run on a WDW-100E machine and hardness on an HBE-3000A tester.

The drawing review is free. Our engineers check which casting process suits the part and suggest where the design could change, once we know what the part must achieve. You decide which changes go into the drawing. If your drawing calls out A357 or EN AC-42200, send the specification for review.

Degassing time per melt
15–20 min
Gravity and tilt-pour alloys
A356, ZL114
Heat treatment
T5/T6 in-house
Tensile testing
In-house, WDW-100E
Floor-standing universal testing machine with a test bar clamped between grips in a bright lab
Tensile testing machine for mechanical properties
Front of a benchtop optical emission spectrometer with sample stand and two buttons, blue curtain behind
Optical emission spectrometer for alloy composition checks

A356 vs A357: buyer questions

Is A357 stronger than A356?

Yes, in static strength. Under ASTM B108/B108M-19, A357.0-T61 test bars have minimums of 310 MPa (45 ksi) tensile and 250 MPa (36 ksi) yield, against 260 MPa (38 ksi) and 180 MPa (26 ksi) for A356.0-T61. Minimum elongation is 3% against 4% (SI table) or 5% (inch-pound).

What is the equivalent of A357?

The closest grades are EN AC-42200 (AlSi7Mg0.6) in EN 1706 and ZL114A in GB/T 1173-2013. Neither is identical: EN 1706 pairs 42200 with 357.0, which has no beryllium addition, and ZL114A allows up to 0.07% beryllium and 0.75% magnesium.

Does A357 contain beryllium?

Registered A357.0 contains 0.04–0.07% beryllium. E357.0 and F357.0, both registered in 2001, cap it at 0.002%. F357.0 keeps the A357 magnesium range; E357.0 holds magnesium at 0.55–0.6%.

Is A356-T6 the same as A356.0-T61?

Not in ASTM B108. For permanent-mold castings, B108/B108M-19 lists A356.0 only as T61 (260 / 180 MPa / 4%, SI). Its T6 row belongs to 356.0, a different alloy with up to 0.6% iron, at 230 / 150 MPa / 3%. ASTM B26 lists A356.0-T6 for sand castings. If a drawing says "A356-T6 to B108," ask which row applies.

Is ZL101A the same as A356?

It is the closest Chinese grade, not an identical one. ZL101A requires 0.08–0.20% titanium. Its GB/T 1173-2013 metal-mold T6 minimum is 295 MPa tensile and 3% elongation, with no yield minimum.

Sources

  • Aluminum Association, Pink Sheets, revised August 2025.
  • ASTM B108/B108M-19 and B26/B26M-18; active editions ASTM B108/B108M-25 and B26/B26M-25.
  • EN 1706:2020+A1:2021; GB/T 1173-2013.
  • IARC, List of Classifications: beryllium and beryllium compounds, Group 1.
  • Chen et al., China Foundry, 2010; Tzeng et al., Metals, 2018; Rio Tinto foundry alloys catalog, 2019.

Send your drawing with the alloy specification

Include the standard and edition, the temper, any yield requirement, the test basis and the zones where properties apply. Submit the RFQ details, then email your drawing for review.

Send your drawing →

Linda

Export Sales

linda@ningbobohua.com